A tensile test of SAE 1020 steel produced the data below (Data available for download. 1) 2experiment are as follows:
Extension [mm] |
Load [kN] |
0.00 |
0.00 |
0.09 |
1.9 |
0.31 |
6.1 |
0.47 |
9.4 |
2.13 |
11.0 |
5.05 |
11.7 |
10.50 |
12.0 |
16.50 |
11.9 |
23.70 |
10.7 |
27.70 |
9.3 |
34.50 |
8.1 |
Plot a graph of Load vs Extension, annotate your graph.